Look at the side of any steel valve and you will find a few characters cast or stamped into the body. WCB, CF8M, A105, LCC, 1.4408. To a buyer they look like part numbers. To an engineer they define the chemistry, strength, temperature range and pressure rating of the most important pressure retaining part on the valve. Reading them correctly takes a little practice and saves a great deal of trouble when a valve arrives on site with a body that does not match the specification.
Where the marking comes from
Marking of steel valves follows MSS SP-25, which sets out what must appear on the body and the identification plate, including manufacturer, pressure class, body material, size, flow direction where relevant and trim identification. ASME B16.34 then ties the body material to a pressure and temperature rating by placing each material in a group. Group 1.1 contains the common carbon steels such as A105 forgings and A216 WCB castings, which share one rating table. Group 2.2 contains the type 316 materials, CF8M castings and F316 forgings among them.
The marking is shorthand for a specification. WCB on its own means grade WCB of ASTM A216, and that standard, not the three letters, defines the chemistry, mechanical tests, heat treatment and weld repair rules. Read the code first, then go to the governing standard for the detail.
Cast carbon and alloy steels
Most cast steel valve bodies are made to one of three ASTM specifications.
- ASTM A216 covers carbon steel castings suitable for fusion welding and high temperature service. The grades are WCA, WCB and WCC. W stands for weldable, C for carbon and the last letter is the grade. WCB is the workhorse of general process valves and WCC a slightly stronger variant.
- ASTM A352 covers castings for low temperature service, with grades such as LCB and LCC. The L marks low temperature, and these grades are impact tested well below zero. LCC is the usual choice where a carbon steel valve has to stay tough in a cold climate or downstream of a gas letdown.
- ASTM A217 covers alloy steel castings for high temperature service. WC6 is 1.25 chromium, 0.5 molybdenum, WC9 is 2.25 chromium, 1 molybdenum, C5 is 5 chromium, 0.5 molybdenum and C12 is 9 chromium, 1 molybdenum. C12A is the modified 9 chromium grade with vanadium and niobium for creep strength. These are the materials for superheated steam and hot hydrocarbon service.
The trap is that A216 and A352 grades look interchangeable on paper and are not. A WCB body has no guaranteed toughness at low temperature, and the minimum design metal temperature rules in ASME B31.3 can rule it out. On any service that can cool below ambient, through Joule Thomson cooling across a let down valve or through autorefrigeration of a liquefied gas on depressurisation, check the code letter before anything else.
Reading cast stainless designations
Cast stainless grades in ASTM A351, and in related specifications for corrosion and heat resistant castings, use a system that originated with the Alloy Casting Institute. It looks cryptic at first but it follows rules.
- The first letter is C for corrosion resistant service or H for heat resistant service.
- The second letter indicates the approximate nickel content, moving through the alphabet as nickel rises. F covers the 19 chromium, 9 to 12 nickel family that corresponds to wrought 304 and 316.
- The number gives maximum carbon in hundredths of a per cent, so 8 means 0.08 per cent and 3 means 0.03 per cent.
- Any final letters indicate added elements. M is molybdenum, N is nitrogen and C is niobium, formerly called columbium.
So CF8 is the cast counterpart of 304, CF8M of 316, CF3M of 316L and CF8C of the niobium stabilised 347. CN7M is a high nickel alloy chosen for sulphuric acid. Duplex castings have their own grade numbers, typically in ASTM A890 or A995, where 4A is a 22 chromium duplex and 5A a 25 chromium super duplex.
Cast and wrought grades are counterparts, not twins. CF8M usually contains some ferrite in its austenitic matrix, which helps castability and resistance to hot cracking but can lower corrosion resistance in some media and makes the casting slightly magnetic. A buyer who puts a magnet on a CF8M valve and feels a pull has not necessarily found a fake.
Forgings and European numbers
Small bore and high pressure valves are often forged. The matching ASTM specifications are A105 for carbon steel, A350 LF2 for low temperature carbon steel and A182 for alloy and stainless forgings. A182 grades carry F numbers that mirror the wrought grades, F304, F316 and F316L for austenitic stainless, F11 and F22 for chromium molybdenum steels and F51 and F53 for duplex and super duplex. The F simply means forged.
European valves often carry EN material numbers, with EN 1503 listing the materials used for valve shells. The numeric form is the most reliable to read. 1.0619, named GP240GH, is the usual cast carbon steel and broadly comparable with WCB. 1.4408, named GX5CrNiMo19-11-2, is the cast 316 and broadly comparable with CF8M. In those names G indicates a casting, X a high alloy steel, the first number the carbon content in hundredths of a per cent, and the symbols and numbers that follow the main alloying elements.
| ASTM grade | Product form | Nominal type | EN number, broadly comparable |
|---|---|---|---|
| A216 WCB | Casting | Carbon steel | 1.0619 |
| A217 WC6 | Casting | 1.25 chromium, 0.5 molybdenum | 1.7357 |
| A351 CF8 | Casting | Austenitic, 304 type | 1.4308 |
| A351 CF8M | Casting | Austenitic, 316 type | 1.4408 |
| A351 CF3M | Casting | Austenitic, 316L type | 1.4409 |
| A182 F316 | Forging | Austenitic, 316 type | 1.4401 |
Comparable does not mean identical. Chemistry ranges and test requirements differ, so a substitution between systems needs checking against both standards.
Trim codes and the certificate behind the marking
The body marking says nothing about the parts that see the most wear, the stem, seats and closure member. On API 600 gate valves and similar designs these are described by an API trim number on the identification plate. Trim 8, with a 13 chromium stainless stem and wedge and hard faced seats, is common on carbon steel valves in general hydrocarbon service. Trim 5 has hard facing on both seats and wedge, and trim 12 uses 316 stainless with hard faced seats. Read the trim number as carefully as the body code, because a WCB valve with the wrong trim fails just as surely as one with the wrong body.
The marking only tells you what the manufacturer claims. The proof is the material test certificate, normally to EN 10204 type 3.1, which should carry the same heat number as the body and give the chemical analysis and mechanical test results for that heat. On critical service, add positive material identification with a portable analyser at goods receipt. For sour service, confirm that the materials also meet the hardness limits of NACE MR0175 or ISO 15156, which never appear in the body code.
For background on the organisation behind most of these specifications, the ASTM International entry is a useful start. The valve itself, read correctly, tells you most of the rest.